Generally. . .
100% overflow can be put back into feed cartridges.
Sift powder cake and pitch hard chunks in the trash.
Mix the sifted material with new duraform at a ratio between 25% to 50% virgin. If you run weak laser and low temps, 25% may suffice. If you run a higher laser power and your part cakes are always stiff, 50% may be necessary.
****************************************************
David K. Leigh ph(254) 933-1000
Harvest Technologies fax(254) 298-0125
dkleigh@harvest-tech.com
----- Original Message -----
From: H.Byun
To: rp-ml@bart.lpt.fi
Sent: Tuesday, October 10, 2000 10:25 AM
Subject: powder ratio for SLS 2000
Hi RPer
I express my thank that you gave me information on the laser power.
but, another problem happened. I dont know powder ratio for SLS 2000 ; new : overflow : used.
Can you recommand the suitable powder ratio to me?
Please, let me know it.
thank you